A post-tensioned slab is concrete squeezed by steel tendons stretched after the pour, so a 9 inch flat plate can span about 30 feet. Crews stress the tendons 3 to 5 days after placement, and nobody should drill it blind.
Key takeaways
- A 30 by 33 ft bay needs roughly a 9 in post-tensioned flat plate, a span-to-depth ratio near 44, per PTI Technical Note 22 (October 2023).
- ACI 318 requires an average effective precompression of at least 125 psi in two-way post-tensioned slabs (Section 8.6.2.1), and the California State University peer-review guideline calls 150 to 175 psi optimum.
- The CSU Guidelines for Post-Tensioned Concrete Structures (2018) require stressing within 3 to 5 days of the pour and prohibit drilling unless tendons are marked, x-rayed or photographed first.
- The University of Houston Section 03 38 00 (rev. January 29, 2018) bars stressing below 3,000 psi and accepts measured elongations within 7 percent of calculated.
- In a 2021 City of Tampa garage repair bid, fixing one broken tendon was priced at $500 to $4,470, with a $1,763.33 unit price from the low total bidder (bid tab 21-C-00036).
What is a post-tensioned slab and how do unbonded tendons work?
A post-tensioned slab is a cast-in-place concrete slab reinforced with high-strength steel strands that are tensioned after the concrete hardens, then locked off at anchors cast into the slab edges. In U.S. buildings the usual system is the unbonded single-strand tendon: a 270,000 psi strand (ASTM A416, per UH Section 03 38 00) coated in corrosion-inhibiting grease inside a plastic sheath, so the strand never bonds to the concrete.
Before the pour, crews drape each tendon high over the columns and low at midspan. When the jack pulls the strand at the stressing anchor, the curved tendon pushes up on the slab between supports and squeezes it lengthwise. That upward push carries part of the dead load, which is why the slab can be thinner than a rebar-only slab. CSU’s guideline asks designers to balance at least 65 percent and no more than 125 percent of the concrete weight.
Where you find them in commercial work: suspended floors in parking garages, office and hotel flat plates, and multifamily podium decks. The City of Seattle’s Director’s Rule 14-2014 credits the system with up to 40 percent less concrete and 75 percent less reinforcing steel than conventional framing, plus fewer construction joints and a lower building profile. The same mechanism appears in slabs on ground over expansive clay, covered further down.
How thick is a post-tensioned slab and how far can it span?
Published commercial examples put a post-tensioned flat plate at about 9 inches for 30 ft column bays, a span-to-depth ratio of 40 to 44. Heavy loads push the slab thicker: a food storage floor with live loads up to 600 psf used 14 inches plus drop panels. Ask your engineer for the governing span-to-depth ratio before fixing floor-to-floor heights.
| Published example | Bay | Slab thickness | Span to depth | Source |
|---|---|---|---|---|
| Typical office panel, PT flat plate | 30 x 33 ft | About 9 in | 44 (33 ft x 12 / 9 in) | PTI Technical Note 22, Section 9.1 (2023) |
| Same building with band beams (Fort Lauderdale, built from 2007) | 30 x 33 ft | 8 in slab, 17 in bands | 50 on the slab alone | PTI Technical Note 22, Section 9.1 |
| Research prototype, high-rise span | 30 x 30 ft, 7.5 ft cantilever | 9 in | 40 | PTI Technical Note 22, Section 10 |
| Food storage facility, live load 100 to 600 psf | 29.7 x 29.7 ft | 14 in, drops to 31 in | 25 | PTI Technical Note 22, Section 9.2 |
| Conventional flat plate, interior panel (contrast) | 28 ft clear span | 10.2 in code minimum | 33 on clear span | ACI 318-19 Table 8.3.1.1 |
PTI Technical Note 22 says its analytical examples use span-to-depth ratios slightly less than 45. CSU tells designers to meet or exceed Table 9.3 of the Post-Tensioning Manual, 6th Edition, and to switch from shear studs to column caps once slabs reach 10 inches. Garage decks exposed to deicing salt need at least 5,000 psi under ACI 318 exposure class F3, as our guide to concrete psi requirements explains.
What does ACI 318 require for a post-tensioned slab?
ACI 318, the concrete code adopted by the International Building Code (IBC), sets the minimum squeeze, tendon spacing and column integrity tendons for a post-tensioned slab. Owner specifications then add tighter limits on pull length, placing tolerance and stressing strength. The table lists the rules a reviewer checks first, with the clause behind each.
| Rule | Value | Source |
|---|---|---|
| Average effective precompression, two-way slabs | 125 psi minimum | ACI 318 Section 8.6.2.1, cited in CSU item 3 and PTI TN 22 |
| Practical precompression range | 150 to 175 psi optimum, 250 psi maximum | CSU item 14 |
| Integrity tendons through columns | Shown on drawings; PTI notes a minimum of two tendons through the column each way | ACI 318 Section 8.7.5.6.1 (CSU item 2); PTI TN 22 |
| Uniform tendon spacing | Lesser of 8 times slab thickness or 5 ft (UH spec: 8h, max 54 in) | CSU item 6; UH 3.1.D |
| Tendon encapsulation | Required; exposed strand details not permitted | ACI 318 Sections 20.6.3.1 to 20.6.3.3 (CSU item 1) |
| Pull length | 125 ft from one end, 250 ft from two ends | UH 3.4.D; CSU item 16 |
| Vertical placing tolerance | Plus or minus 1/4 in (slabs 8 in or less), 3/8 in (8 to 24 in) | UH 3.1.C |
| Cover to anchor wedge cavity | 2 in minimum at slab edge | UH 3.2.A.2 |
| Strand | ASTM A416 low-relaxation, 270,000 psi ultimate | UH 2.1.A |
| Broken tendons left unreplaced | Total force loss 2 percent maximum | UH 3.4.H |
How much force that means: at the 125 psi floor, one foot of a 9 inch slab (108 square inches) needs 13,500 lb of effective force, so a 30 ft wide panel needs 405,000 lb. One 1/2 inch strand of 0.153 square inches at 270,000 psi breaks at about 41,300 lb, so even at full ultimate strength it takes 10 strands; real designs carry more because effective force after losses sits well below ultimate.
| Step | Input | Result |
|---|---|---|
| Area per foot of 9 in slab | 9 in x 12 in | 108 sq in |
| Force per foot at ACI minimum | 108 sq in x 125 psi | 13,500 lb |
| Force across a 30 ft panel | 13,500 lb x 30 | 405,000 lb |
| Same panel at CSU optimum | 108 x 150 to 175 psi x 30 | 486,000 to 567,000 lb |
| Strand breaking strength | 0.153 sq in x 270,000 psi | 41,310 lb |
| Strands at 125 psi if each carried its full ultimate | 405,000 / 41,310 | 9.8, so 10 or more |
When are the tendons stressed, and in what order?
Tendons in a commercial post-tensioned slab are stressed once field-cured cylinders show the concrete has reached the stressing strength on the drawings, at least 3,000 psi in the University of Houston specification, and within 3 to 5 days of the pour under the CSU guideline. Stressing early limits shrinkage cracking; stressing too early can crush concrete behind the anchors.
- Hold the pre-construction meeting. Seattle requires the general contractor, engineer of record, tendon placer, supplier, concrete supplier, finisher and testing agency; UH requires it at least 30 days before PT work starts.
- Inspect tendons and rebar before the pour. Seattle requires at least 4 hours between inspector sign-off and concrete placement, and at least two special inspectors on the pour.
- Cure test cylinders on the deck. Seattle Rule 13 bars using lab-cured cylinders to release stressing.
- Stress in sequence: temperature tendons, continuous slab tendons, added slab tendons, then beam and girder tendons (UH 3.4.F).
- Measure every elongation to 1/8 inch and send records to the engineer by the next working morning (Seattle Rules 16 and 17); UH accepts results within 7 percent of calculated.
- Cut tails 24 to 48 hours after engineer approval (Seattle Rule 18), at least 1/2 inch inside the concrete face (UH 3.5.A), then cap and grout the pockets.
- Close pour strips no sooner than 30 days after the second pour for plans up to 250 ft, or 60 days for larger plans (CSU item 8).
Stressing is a federal safety item. OSHA 29 CFR 1926.701(c) keeps everyone except essential crew from standing behind the jack and requires signs and barriers around the stressing area. Seattle Rule 15 goes further and clears the deck of anyone not directly involved, because a tendon that breaks during stressing can cause serious injury. Curing strength gain by day is covered in our guide to concrete curing time.
Can you drill or core a post-tensioned slab?
Only after the tendons are located. CSU item 24 prohibits drilling into a post-tensioned slab unless tendon locations are marked, the slab has been x-rayed, or the tendons were photographed before the pour, and Seattle bars any drilling into the deck after placement. A cut tendon loses force over its full length, not just at the hole.
Because the drape runs from near the top over columns to near the bottom at midspan, no depth in the slab is automatically safe. The UH specification keeps tendons at least 6 inches from openings and limits horizontal sweeps to a radius of 480 strand diameters. CSU also limits shot pins to the concrete cover over the tendons and requires Schedule 40 steel sleeves, not PVC, near anchors.
| Locating method | How it works | Rule or limit | Source |
|---|---|---|---|
| Pre-pour photos or drone survey | Photograph tendons on chairs before concrete covers them | Accepted by CSU before drilling | CSU items 24 and 29 |
| Permanent slab marking | Paint or inserts mark tendon bands on the soffit | CSU asks for it where future changes are expected | CSU item 29 |
| Ground-penetrating radar (GPR) | Radar scan from one face, no radiation | Confirm against shop drawings; no code depth standard | Industry practice |
| X-ray radiography | Source on one face, film on the other | Licensed radiographers and a cleared area under NRC rules | 10 CFR Part 34 |
CSU item 18 calls de-tensioning a very dangerous operation and tells designers to avoid requiring it. If a renovation needs a new shaft or stair opening through a post-tensioned slab, budget a structural engineer to design the cut and re-anchoring; our structural engineer cost guide gives fee ranges.
Post-tensioned vs conventionally reinforced slab: which costs less?
A post-tensioned slab uses less concrete and steel, but adds strand, anchors, a stressing crew and inspection. At a 30 ft bay, the concrete saving against a code-minimum conventional flat plate is about 3.3 cubic yards per bay, worth roughly $0.62 per square foot at a 2026 public bid price. The larger savings are floor height and dead load.
| Factor | Post-tensioned slab | Conventionally reinforced slab | Source |
|---|---|---|---|
| Thickness, 30 ft bay | About 9 in | 10.2 in interior, 11.2 in exterior without edge beam (code minimum, 28 ft clear) | PTI TN 22; ACI 318-19 Table 8.3.1.1 |
| Concrete and rebar | Up to 40 percent less concrete, 75 percent less rebar | Baseline | Seattle DR 14-2014 |
| Crack control | Precompression 125 psi minimum keeps slab in compression | Relies on bonded bars; see our rebar sizes guide | ACI 318 Section 8.6.2.1 |
| Schedule | Stress at 3 to 5 days; pour strips wait 30 to 60 days | No stressing step | CSU items 8 and 27 |
| Later penetrations | Locate tendons first; drilling prohibited without it | Scan for bars, cutting a bar is local | CSU item 24 |
| Special inspection | Tendon placement, pour, stressing and cut-off | Rebar placement and pour | Seattle DR 14-2014 |
Worked example for one interior 30 by 30 ft bay (900 square feet). The conventional thickness uses ACI 318-19 Table 8.3.1.1 for an interior panel without drop panels and 60,000 psi bars, clear span divided by 33, with an assumed 24 inch column. The concrete price is the $169 per cubic yard 4,000 psi low bid in Tioga County, NY (opened January 15, 2026), delivered material only.
| Line | Post-tensioned | Conventional |
|---|---|---|
| Clear span | 28 ft | 28 ft |
| Thickness | 9 in (PTI TN 22) | 28 x 12 / 33 = 10.2 in |
| Concrete per bay | 900 x 0.75 / 27 = 25.0 cu yd | 900 x 0.85 / 27 = 28.3 cu yd |
| Concrete cost at $169 per cu yd | $4,225 | $4,783 |
| Difference | 3.3 cu yd and $558 per bay, about $0.62 per sq ft, plus 1.2 in less height per floor | |
The ACI value is a minimum that lets designers skip a deflection calculation; a 30 ft conventional flat plate often ends up thicker or with drop panels, which widens the gap. For slab-on-ground pricing by thickness, see our concrete slab cost per square foot guide.
What does post-tensioned slab work cost in public bids?
We found no public bid tabulation or federal award that prices new post-tensioned slab work as a separate per-square-foot line; garages are usually bid as one structural package. Repair work is itemized: the City of Tampa’s June 22, 2021 garage repair bid priced broken tendon repair at $500 to $4,470 each across four bidders.
| Item (Tampa bid 21-C-00036, Rivergate and other garages) | Unit | Qty | Bid range | Median of 4 | Median x 1.354 (2026) |
|---|---|---|---|---|---|
| Repair broken PT tendons | Each | 12 | $500 to $4,470 | $2,632 | $3,563 |
| Repair PT tendon sheathing | Sq ft | 80 | $35 to $150 | $133 | $180 |
| Re-grout PT tendon pockets | Each | 60 | $93 to $141 | $110 | $149 |
| Post-tensioned beam repair (Rivergate) | Sq ft | 25 | $175 to $288 | $206 | $278 |
| Non-post-tensioned beam repair (Fort Brooke, contrast) | Sq ft | 70 | $95 to $278 | $176 | $238 |
The 1.354 factor is the change in the BLS producer price index for concrete contractors, nonresidential building work (PCU23811X23811X), from 145.919 in September 2021 to a preliminary 197.561 in September 2026. Quantities were small (12 tendons), so mobilization is likely spread into the unit prices; expect a single tendon call-out to cost more.
What should an owner inspect on a post-tensioned deck?
Post-tensioned slabs fall under the IBC special inspection program, and Seattle spells out the checkpoints: tendon placement, the pour, stressing, cut-off and pocket grouting. An owner or owner’s representative can ask for these records at each stage. Our special inspections guide covers who hires the inspector.
| Stage | What to check | Pass condition | Source |
|---|---|---|---|
| Delivery | Mill certificates and 6 ft strand samples per shipment | Samples held by testing agency until final letter | Seattle Rule 5 |
| Before pour | Sheathing tears, chair spacing, profile heights | Supports at 4 ft maximum; repairs watertight | UH 3.1.E and 3.1.G |
| Pour | Slump at chute, no added water beyond ticket | Ticket states gallons allowed per load | Seattle Rules 7 and 11 |
| Stressing | Calibrated ram and gauge, one inspector per ram | Elongation within 7 percent of calculated | UH 3.4.C and 3.4.E; Seattle Rule 14 |
| Cut-off | Tail length and caps | Cut 1/2 in inside face, capped within 24 h | UH 3.5.A and 3.5.B |
| Closeout | Pockets grouted, as-built tendon record | Engineer acceptance letter received | Seattle Rule 4; CSU item 29 |
When is post-tensioning used for a slab on ground?
On expansive clay, IBC Section 1808.6.2 lets designers build a slab-on-ground foundation to the PTI DC10.5 standard or the WRI/CRSI method instead of deep foundations. The tendons tie the slab into one stiff mat that rides soil swell. The trigger is the expansion index in your geotechnical report; plasticity and swell values feed the design.
Residential contrast: house slabs use the same tendons, but warehouse rack, forklift and dock loads need their own design check.
Should your project use a post-tensioned slab?
Choose post-tensioning when column bays near 30 ft, a flat soffit and floor height matter, as in garages and podium decks. Choose conventional reinforcing when tenants will core the slab often and nobody will keep tendon maps. Long plans over 350 ft still work with a permanent expansion joint.
| If | Then | Source |
|---|---|---|
| Slab on ground over expansive soil | Design to PTI DC10.5 or WRI/CRSI | IBC 2021 Section 1808.6.2 |
| Supported bays near 30 ft, flat soffit wanted | Price a PT flat plate around 9 in | PTI TN 22 |
| Bays well under 30 ft and height is not tight | Price conventional; the code minimum may be close to PT thickness | ACI 318-19 Table 8.3.1.1 |
| Frequent future coring or anchors | PT only with marked or photographed tendons; else conventional | CSU items 24 and 29 |
| Plan dimension over 250 ft | Allow a 60 day pour strip delay in the schedule | CSU item 8 |
| Plan dimension over 350 ft | Add a permanent expansion joint | CSU item 8 |
| Slab 10 in or thicker | Use column caps, not shear studs | CSU item 26 |
Before fixing a garage column grid against the 30 ft PTI examples, check stall and aisle sizes in our parking space dimensions guide.
What do common guides get wrong about post-tensioned slabs?
Several page-one guides were written for houses or for markets outside the U.S. and carry numbers that do not fit a commercial post-tensioned slab. The table sets three claims against the primary document.
| What a guide says | What the primary source says | Source |
|---|---|---|
| A top-ranking general guide says concrete cures 20 to 25 days to reach 75 percent strength before stressing | Stress within 3 to 5 days, once field-cured cylinders reach the specified strength | CSU item 27; UH 3.4.B |
| Residential guides cite stressing at 2,000 psi | Commercial owner spec: not less than 3,000 psi unless drawings say otherwise | UH 3.4.B |
Slab design starts from the soil bearing capacity in the geotechnical report and the vapor barrier under the slab.
How we compiled this
We read 7 primary documents in November 2026: PTI Technical Note 22, the CSU Seismic Review Board post-tensioning guideline, the University of Houston Section 03 38 00, Seattle Director’s Rule 14-2014, OSHA 29 CFR 1926.701, the City of Tampa bid tab 21-C-00036 and the BLS PPI series, plus the Tioga County bid already used on our site. ACI 318-19 and IBC clauses are cited as quoted in those documents or from the code tables. We did not test, design or price any slab ourselves.
Frequently asked questions
How thick is a post-tensioned slab in a parking garage?
Published examples put a post-tensioned flat plate at about 9 inches for 30 ft column bays, a span-to-depth ratio of 40 to 44 (PTI Technical Note 22, 2023). Band-beam layouts can drop the slab to 8 inches with 17 inch bands. Heavy storage loads pushed one 29.7 ft bay to 14 inches with drop panels. Your engineer sets the final thickness from loads and fire cover.
How long after pouring are post-tensioned tendons stressed?
The CSU post-tensioning guideline requires stressing within 3 to 5 days of the pour to limit shrinkage cracking. The release is strength, not days: the University of Houston specification requires at least 3,000 psi unless the drawings say otherwise, and Seattle Director’s Rule 14-2014 only accepts field-cured cylinders, never lab-cured ones, to prove that strength.
Can I drill into a post-tensioned slab to install an anchor?
Not until the tendons are located. CSU item 24 prohibits drilling unless tendon locations are marked, the slab is x-rayed, or pre-pour photos exist, and it limits shot pins to the cover over the tendons. Tendons run near the top over columns and near the bottom at midspan, so no depth is automatically safe. Ask the owner for the as-built tendon drawings first.
What happens if a tendon is cut?
An unbonded tendon loses its force along its whole length, not just at the cut, because the strand is greased and free inside its sheath. The University of Houston specification limits unreplaced broken tendons to 2 percent of a member’s total prestress force. In a 2021 City of Tampa repair bid, replacing one broken tendon was priced from $500 to $4,470.
Is a post-tensioned slab cheaper than a conventional slab?
It uses less material: Seattle Director’s Rule 14-2014 cites up to 40 percent less concrete and 75 percent less reinforcing steel. At a 30 ft bay, the concrete saving against a code-minimum conventional flat plate is about 3.3 cubic yards per bay, roughly $0.62 per square foot at a 2026 Tioga County bid price, before strand, anchors and stressing labor.
What is the minimum precompression in a post-tensioned slab?
ACI 318 Section 8.6.2.1 requires an average effective precompression of at least 125 psi in two-way post-tensioned slabs. The California State University guideline treats 150 to 175 psi as optimum and caps flat plates at 250 psi. For a 9 inch slab, 125 psi equals 13,500 lb of effective force per foot of width.
Sources
- Technical Note 22: Dual-Banded Post-Tensioning Tendon Layout, Post-Tensioning Institute, October 2023, accessed November 15, 2026
- CSU Guidelines for Post-Tensioned Concrete Structures, California State University Seismic Review Board, April 27, 2018, accessed November 15, 2026
- Section 03 38 00 Post-Tensioned Concrete, University of Houston Master Construction Specifications, rev. January 29, 2018, accessed November 15, 2026
- Director’s Rule 14-2014, Post-Tensioned Concrete Installation and Special Inspection Requirements, City of Seattle DPD, effective October 27, 2014, accessed November 15, 2026
- 29 CFR 1926.701 General requirements (concrete and masonry), OSHA via eCFR, accessed November 15, 2026
- 10 CFR Part 34 Industrial radiography, U.S. NRC via eCFR, accessed November 15, 2026
- ACI 318-19 Building Code Requirements for Structural Concrete, American Concrete Institute, 2019, accessed November 15, 2026
- 2021 International Building Code, Chapter 18, International Code Council, accessed November 15, 2026
- Bid 21-C-00036 Parking Garage Improvements itemized bid tab, City of Tampa Contract Administration, opened June 22, 2021, accessed November 15, 2026
- Portland cement concrete bid tabulation, Tioga County, NY Public Works, opened January 15, 2026, accessed November 8, 2026
- PPI PCU23811X23811X Concrete contractors, nonresidential building work, U.S. Bureau of Labor Statistics, accessed November 8, 2026